· Description: SJ605 is a fluorine-based high-basicity sintered flux with a particle size of 2.0-0.45mm (10-40 mesh). The flux is metallurgical neutral, has good welding processability, stable arc, easy slag removal, beautiful weld formation, high purity of weld metal and high low temperature impact toughness.
· Application: It can weld fine grain low temperature steel and high strength structural steel with appropriate welding wire, such as low temperature pressure vessels, oil storage tanks and oil and gas pipelines, marine engineering, nuclear industry, etc.
· The test results of SJ605 matching different welding wires are listed below:
· Mechanical properties of deposited metal (GB / T F48P10-ENi3, equivalent to AWS F7P15-ENi3)
Pilot projects | tensile strengthR m (MPa) | Yield StrengthR eh (MPa) | ElongationA (%) | AKV(J) |
-101℃ | ||||
guarantee value | 480-660 | ≥400 | ≥20 | ≥27 |
Detection value | 536 | 477 | 31 | 156、112、125、150、119/131 |
· Deposition metal flux composition (%)
project | C | Mn | Si | S | P | Ni | Cr |
Specified value | ≤0.12 | ≤1.60 | ≤0.80 | ≤0.025 | ≤0.025 | 2.80-3.80 | ≤0.15 |
Example value | 0.054 | 0.983 | 0.272 | 0.005 | 0.007 | 2.921 | 0.038 |
project | Cu | Co | B | V | As | Sh | Sb |
Limit value | ≤0.35 | ≤0.03 | — | ≤0.02 | ≤0.01 | ≤0.01 | ≤0.01 |
Example value | 0.063 | 0.006 | <0.001 | 0.004 | 0.006 | 0.006 | 0.001 |
· Mechanical properties of deposited metal (GB / T F48P7-H09MnNiDR, equivalent to AWS F7P10-ENi3)
Pilot projects | tensile strengthR m (MPa) | Yield StrengthR eh (MPa) | ElongationA (%) | AKV(J) |
-72℃ | ||||
guarantee value | 480-660 | ≥400 | ≥20 | ≥27 |
Detection value | 585 | 500 | 26 | 96、150、150、129、131/137 |
· Chemical composition of deposited metal (%)
project | C | Mn | Si | S | P | Cr | Ni | Mo | Cu |
Specified value | ≤0.10 | ≤1.25 | ≤0.5 | ≤0.010 | ≤0.015 | ≤0.15 | 2.80-3.80 | --- | ≤0.35 |
Example value | 0.061 | 0.794 | 0.270 | 0.002 | 0.008 | 0.089 | 2.864 | 0.017 | 0.127 |
· Mechanical properties of deposited metal (GB / T F76P6-H08Mn2Ni3MoA <H3NiMoCr>, equivalent to AWSF11P8-EF5)
Pilot projects | tensile strengthR m (MPa) | Yield StrengthR eh (MPa) | Elongation A (%) | AKV(J) |
-62℃ | ||||
guarantee value | 760-900 | ≥680 | ≥15 | ≥27 |
Detection value | 808 | 740 | 22 | 112、97、104、99、101/101 |
· Chemical composition of deposited metal (%)
project | C | Mn | Si | S | P | Cr | Ni | Mo | Cu |
Specified value | ≤0.17 | 1.20-1.80 | ≤0.80 | ≤0.030 | ≤0.030 | ≤0.65 | 2.00-2.80 | 0.30-0.80 | ≤0.50 |
Example value | 0.077 | 1.565 | 0.264 | 0.002 | 0.010 | 0.346 | 2.101 | 0.632 | 0.087 |
· Mechanical properties of deposited metal (GB / T F48P2-H13CrMoA <HCr1Mo>, equivalent to AWS F7P0-EB2)
Pilot projects | tensile strengthR m (MPa) | Yield StrengthR eh (MPa) | ElongationA (%) | AKV(J) |
-20℃ | ||||
guarantee value | 480-660 | ≥400 | ≥22 | ≥27 |
Detection value | 554 | 462 | 32 | 198、120、161、192、153/169 |